1. Flow Marks

Problem

Flow marks result from material's physical properties. The material's flow trace, especially when the filler (including color master) isn't well - dispersed, shows as a visible pattern, like a river's flow, especially in areas with inconsistent thickness.

Solutions

  • Adjust Injection Speed: Use multi - stage injection. For uneven - wall - thickness parts, increase speed in thin - wall areas and decrease in thick - wall areas. For common ABS parts, control filling speed at 30 - 50 mm/s.

  • injection mould

  • Control Mold Temperature: Use a mold temperature controller. Different thermoplastics have different optimal mold temperature ranges. For PP, it's 40 - 60 °C; for PC, 80 - 100 °C. Set temperature sensors inside the mold for real - time monitoring.

  • injection mould

  • Optimize Gate Design: Redesign the gate according to part structure and material. Increase gate size to reduce melt flow rate and choose a proper gate location. For flat parts, a side gate in the middle of the length might be suitable.

2. Tiger Skin Pattern

Problem

The material's physical properties, like in modified automotive plastics with base materials and rubber particles, cause a wavy ejective appearance. Strong - elasticity plastics and color - master coloring issues can also lead to this pattern.

injection mould

Solutions

  • Materials: Strictly control material quality, use the same - batch stable materials and conduct random inspections. Optimize additive use and ensure uniform dispersion.

  • Mold: Optimize the gate by adjusting size and position. Improve the runner by polishing, controlling size, and checking hot - runner heating elements.

  • Injection Molding Process: Stabilize injection parameters, control speed fluctuation within ±5% with closed - loop control. Use a high - precision temperature controller, especially for complex molds with partition temperature control.

3. Trapped Air

Problem

Trapped gas, which differs from gas marks, can't move with the fluid at the end or in corners. Compressed gas raises temperature, causing oxidation and possible burning and yellowing on the product surface. Symptoms include wavy patterns, material shortage, yellowing, and blackening.

Solutions

  • Optimize Exhaust System: Check and clean vent holes and slots. Add an exhaust tank (width 0.02 - 0.05 mm, depth 0.01 - 0.03 mm) in gas - trapping areas. Use ventilated steel for better exhaust.

  • Improve Mold Structure: Simplify complex molds to reduce gas - trapping. Use vacuum exhaust to extract air before injection.

  • injection mould

4. Cold Material

Problem

Cold material forms for two main reasons: the front - end material solidifies in the cycle and is pushed by the back - end material, or there are leftover scraps from the last mold (like shovel - glue leftovers, gate wire - drawing scraps, or electrostatic - adsorbed scraps on the parting surface). This causes an illusion of gas marks on the product surface.

Solutions

  • Adjust Barrel Temperature: Set each barrel section's temperature according to the plastic material. For cold - material - prone materials like nylon (PA), set the starting temperature at 240 - 260 °C. Ensure a proper temperature gradient for uniform heating.

  • Optimize Injection Molding Machine Start - up: Before restarting, pre - plasticize to remelt potential cold - material blocks. Set a preheating program to rotate the screw and increase barrel temperature.

  • Improve Runner System Design: Optimize the flow path by shortening its length and increasing its diameter (e.g., from 3 mm to 4 mm for small parts). Regularly check and maintain hot - runner heating elements.

  • Shorten Injection Cycle: Optimize injection speed and pressure - holding time. Increase injection speed and adjust pressure - holding time to reduce melt residence time in the runner and gate, especially for thin - wall parts.

injection mould


Home
Product
News
Contact
主站蜘蛛池模板: 国产精品成人永久在线四虎 | 一本久久a精品一区二区| 欧美激欧美啪啪片免费看| 日日碰狠狠添天天爽五月婷| 国产亚洲精品字幕在线观看 | 亚洲日韩欧美在线成人| 国产精品永久免费| 国产亚洲精品久久yy50| 久久综合精品国产丝袜长腿| 亚洲国产成人精品无码区在线网站| 在线 欧美 中文 亚洲 精品| 国产欧色美视频综合二区| 中国超帅年轻小鲜肉自慰| av午夜福利一片免费看久久| 日韩视频中文字幕精品偷拍| 潮喷大喷水系列无码| 欧美人牲交免费观看| 国产精品 中文字幕 亚洲 欧美| 欧美性色19p| 人妻少妇精品无码系列| 国产精品女同一区二区在线| 久久无码av一区二区三区| 午夜福利视频网站| 亚洲国产成人久久综合碰碰| 国内精品久久久久国产盗摄| 欧美精品亚洲精品日韩已满十八| 欧美99久久无码一区人妻a片| 国产成a人亚洲精v品无码| 久久久久成人网站| 亚洲国产无套无码av电影| 撕开?吸奶头?进| 成人区精品一区二区不卡av免费| 亚洲国产精品成人天堂| 成人va亚洲va欧美天堂| 亚洲国产成人极品综合| 免费精品99久久国产综合精品| 亚洲国产精品自在拍在线播放蜜臀| 色婷婷在线精品国自产拍| 国产超级va在线观看视频| 久久人人爽人人爽人人片av高清| 久久亚洲国产五月综合网|