久久精品国产国产精-中文字幕久久波多野结衣av-精品久久久久久中文字幕无码vr-亚洲国产一区二区三区波多野结衣-最新国产精品久久精品

Common problem

Precautions for PPS Plastic Injection Molding

2026-02-28 11:10:25 Injection Molding

PPS is a high-temperature engineering plastic with high rigidity, low water absorption, and narrow processing window. It requires strict control of drying, temperature, injection, and cooling to avoid degradation, bubbles, or deformation.

Material Drying

Drying requirements: Use dehumidifying dryers at 120–140℃ for 3–4 hours (trace moisture accelerates degradation).Storage: Seal raw materials in a dry, cool area; use dried material within 2 hours (re-dry if exposed to air).

Barrel Temperature Control

Recommended temperatures: Rear 260–280℃, Middle 290–310℃, Front 300–320℃, Nozzle 300–310℃.Critical notes: Avoid overheating (causes degradation/yellowing) or underheating (poor flow/short shots). Purge with PP/PE before shutdown to prevent carbonization.

injection mould

Mold Temperature Requirements

Standard parts: 120–150℃ (ensures crystallization and dimensional stability).High-precision parts: 150–180℃ (improves rigidity and surface quality).Key rule: Use a mold temperature controller (avoid natural cooling for inconsistent temperatures).

Injection Pressure & Speed

Pressure: Moderate-to-high injection pressure (avoid excessive pressure to reduce internal stress/flash).Speed: Medium-to-high speed (stable filling, no shear overheating).Holding pressure: Minimal pressure to prevent sink marks (high pressure increases warpage).Back pressure: Low (reduce shear heat and material degradation).

Mold & Venting

Venting: Add 0.015–0.02mm deep vents at weld lines/flow ends (prevent burning/trapping gas).Mold steel: Use H13/SKD61/S136 for glass-filled PPS (wear/corrosion-resistant, nitride-treated for longevity).

injection mould

Cooling & Ejection

Cooling: Sufficient cooling time (prevents warpage/cracking from rapid crystallization).Ejection: Balanced ejector layout (avoid local stress); slow ejection speed (prevent chipping of brittle PPS).Draft angles: Increase angles on deep cavities/ribs (prevent sticking/scratching).

Post-Treatment & Quality Control

Annealing: 150–180℃ for 1–2 hours (eliminates internal stress, stabilizes dimensions).Inspection: Reduce temperature for yellowing/bubbles; increase pressure for short shots; lower pressure for flash/warpage.

Safety & Equipment Maintenance

Safety: Ensure good ventilation (PPS releases corrosive gases at high temperatures).Maintenance: Regularly inspect/wear parts (screws, barrels, molds) for glass-filled PPS wear.

injection mould

Home
Product
News
Contact
主站蜘蛛池模板: 欧美日韩人妻精品一区二区在线| 国产精品一久久香蕉国产线看观看| 国产女人精品视频国产灰线| 性刺激视频免费观看| 亚洲色大成网站www永久| 伊人久久大香线蕉av网禁呦| 日本熟妇人妻videos| 亚洲精品国产av天美传媒| 亚洲欧美精品无码一区二区三区| 中日韩va无码中文字幕| 亚洲精品第一国产综合精品| 人妻有码av中文字幕久久琪| 一个人看的www视频免费观看| 国产一区视频一区欧美| 国产亚洲精品自在久久| 久久欧美国产伦子伦精品| 天天躁日日躁狠狠很躁| 亚洲精品无码av中文字幕电影网站| 精品无码人妻一区二区三区| 亚洲精品美女久久久久久久| 国产精品国产三级国产专i| 欲妇荡岳丰满少妇岳| 九九在线精品国产| 国产亚洲精品久久久久久老妇 | 中文字幕日产无码| 精品无人乱码高清在线观看| 国产熟睡乱子伦午夜视频| 国产精品第一二三区久久蜜芽| 国产性夜夜春夜夜爽1a片| 中文乱码字慕人妻熟女人妻| 国色天香精品一卡2卡3卡4| 99国产亚洲精品美女久久久久| 果冻传媒董小宛视频一区| 精品国内自产拍在线播放观看| 国产成人精品亚洲午夜| 久久99国产精一区二区三区| 成年女人永久免费观看视频| 免费国产午夜高清在线视频| 久久精品国产只有精品66| 东京热人妻系列无码专区| 国产综合久久99久久|